QE大規(guī)格H型鋼QElargespecificationHsteel
《QE大規(guī)格H型鋼QElargespecificationHsteel》由會(huì)員分享,可在線閱讀,更多相關(guān)《QE大規(guī)格H型鋼QElargespecificationHsteel(36頁(yè)珍藏版)》請(qǐng)?jiān)谘b配圖網(wǎng)上搜索。
1、Q345E大規(guī)格H型鋼(Q345E large specification H steel) Volume 31, stage 2 In April 2009, Shandong metallurgical April2009 ShandongMetallurgyVol. 31, No. 2 Abstract: time limitation of Q345E large size h-beam way research found that less influence aging on the impact toughness and 40 ℃, using th
2、e energy method to determine the steel brittleness at low temperature Curve, the brittle transition temperature range for - 30 ~ 40 ℃. The analysis of metallographic structure, the macroscopic and microscopic appearance of the fracture and the microscopic appearance of the inclusions The analy
3、sis of electron probe spectroscopy shows that the main causes of low temperature impact toughness are serious banded structure and non-metallic inclusions in steel. Key words: h-shaped steel; Low temperature impact toughness; Aging; Banded structure; inclusions Middle image classification no.
4、: TG113; TG115 literature identification code: A post no. : 1004-4620 (2009) 02-0040-03 Deadline: 2008-12-23 The author: dong changxing, male, born in 1972, graduated from hebei chengde petroleum university in 1994 Technical college industrial analysis major. Now the quality supervision dep
5、artment of lai-steel quality assurance department Be engaged in quality inspection of steel products. 1 introduction The Q345E large specification H shape steel produced by laishan steel factory is at the beginning Fig.5 found to 40 ℃ impact AkV value is low and volatile, However, aft
6、er two weeks or so of aging, the AkV value increased significantly, mostly Several furnaces meet product standard requirements. In order to improve the steel Low temperature impact toughness and shorten aging time, for product storage, hair The conditions of the goods and the port are creat
7、ed, and the steel H section steel is tested in series And test analysis. By means of different aging methods, Hope to find the best way of aging; On the other hand, the macro of impact sample The distribution and morphology of the fracture, microfracture, tissue morphology and inclusions
8、 Analysis can determine the Q345E of large size h-beam and 40 ℃ impact For low reason, the direction of high temperature impact toughness is determined. 2 aging test The technical requirements of steel Q345E large H steel are shown in table 1 and table 2. often The temperature-aging test
9、 combines boiling water bath and oil bath with natural aging In the same way, the adverse conditions of temperature and environmental conditions are carried out. Aging test A total of 3 rounds were conducted, with the furnace number h083-3622q345e as the first The chemical composition and g
10、as content of the test samples were shown in table 3. Table 1 performance requirements The specification/mm is less than or equal to 16 or greater than or equal to 345 BBB 0, 16 ~ 35 sigma/MPa470 ~ 630 delta s / % Acuity 22 akv (to 40 ℃, the longitudinal)/J 27 q345e big h-beam and 40 ℃ or h
11、igher impact toughness is low cause analysis Dong changxing, cheng mei, time zhenming, dong bingcheng, liu hongyan (laiwu steel group co., LTD. Shandong laiwu 271104) ...... ...... ...... Experimental research project standard Internal control C is less than 0.180.13 ~
12、0.17 Si is less than 0.550.15 ~ 0.25 Mn1.0 ~ 1.61.2 ~ 1.4 P = 0.025 is less than or less than 0.025, or 0.025, or 0.025, 0.015 ~ 0.015 ~ 0.025 Table 2 chemical components control % Table 4 impact test data after oil bath Oil bath temperature / ℃ 120150200280340-40 ℃ AkV/J42, 84421 0,18,8
13、106,50,1020,128,4222,20,58 Test temperature Degree / ℃ The normal temperature 30-40 - Constant temperature of 7d1 # 10834322 # 13046133 # 10810144 # 14212105 # 138269 Room temperature of 15d1 # 10444462 # 11838183 # 9634404 # 11216385 # 1301820 Tabl
14、e 6. Time-temperature adverse impact data J Water bath time No bath 30 min45min60min90min The normal temperature 122,92,130116,144,114100,130,128128,120,12696,132,112-30 ℃ 46,24,4826,48,3028,20,1212,22,1840,38,32-40 ℃ 26, 14, 2834, 40, 32, 18, 12, 18, 14, 14, 12, 16 Table 5 w
15、ater bath after the impact test data JC0.178 Si0.214 Mn1.26 P0.009 S0.007 Cr0.024 Nb0.017 Ni0.01 Cu0.014 Al0.005 [O] * 10-654.1 [N] times 10-637.5 Table 3 samples of chemical composition and gas content % The impact test data after oil bath is shown in table 4 (30min oil bath time). The
16、test data of impact test after water bath is shown in table 5 (water bath temperature 100 ℃); Under normal temperature (10 ~ 30 ℃) aging impact test data shown in table 6. From a large number of experimental data, the temperature of normal temperature has a basic impact Is not affected, 15
17、d after aging, and 30 ℃ and 40 ℃ - impact sbent in Paris Improved, below 30 ℃ impact energy as a whole is not high and volatile, this master If it is caused by the release of residual stress; Oil bath or water bath quickly The effect of effect on the impact work has not been significantly b
18、eneficial It is not obvious that the impact work under the temperature of temperature is not obvious To take a water bath or oil bath with the test specimen, and the condition of the permanent temperature of the whole steel 40 Abstract: time limitation of Q345E large size h-beam way rese
19、arch found that less influence aging on the impact toughness and 40 ℃, using the energy method to determine the steel brittleness at low temperature Curve, the brittle transition temperature range for - 30 ~ 40 ℃. The analysis of metallographic structure, the macroscopic and microscopic appearanc
20、e of the fracture and the microscopic appearance of the inclusions The analysis of electron probe spectroscopy shows that the main causes of low temperature impact toughness are serious banded structure and non-metallic inclusions in steel. Key words: h-shaped steel; Low temperature impact tou
21、ghness; Aging; Banded structure; inclusions Middle image classification no. : TG113; TG115 literature identification code: A post no. : 1004-4620 (2009) 02-0040-03 Deadline: 2008-12-23 The author: dong changxing, male, born in 1972, graduated from hebei chengde petroleum university in 1994
22、 Technical college industrial analysis major. Now the quality supervision department of lai-steel quality assurance department Be engaged in quality inspection of steel products. 1 introduction The Q345E large specification H shape steel produced by laishan steel factory is at the beginni
23、ng Fig.5 found to 40 ℃ impact AkV value is low and volatile, However, after two weeks or so of aging, the AkV value increased significantly, mostly Several furnaces meet product standard requirements. In order to improve the steel Low temperature impact toughness and shorten aging time,
24、for product storage, hair The conditions of the goods and the port are created, and the steel H section steel is tested in series And test analysis. By means of different aging methods, Hope to find the best way of aging; On the other hand, the macro of impact sample The distribution and
25、 morphology of the fracture, microfracture, tissue morphology and inclusions Analysis can determine the Q345E of large size h-beam and 40 ℃ impact For low reason, the direction of high temperature impact toughness is determined. 2 aging test The technical requirements of steel Q345E larg
26、e H steel are shown in table 1 and table 2. often The temperature-aging test combines boiling water bath and oil bath with natural aging In the same way, the adverse conditions of temperature and environmental conditions are carried out. Aging test A total of 3 rounds were conducted, with t
27、he furnace number h083-3622q345e as the first The chemical composition and gas content of the test samples were shown in table 3. Table 1 performance requirements The specification/mm is less than or equal to 16 or greater than or equal to 345 BBB 0, 16 ~ 35 sigma/MPa470 ~ 630 delta s / %
28、 Acuity 22 akv (to 40 ℃, the longitudinal)/J 27 q345e big h-beam and 40 ℃ or higher impact toughness is low cause analysis Dong changxing, cheng mei, time zhenming, dong bingcheng, liu hongyan (laiwu steel group co., LTD. Shandong laiwu 271104) ...... ...... ...... Experimental re
29、search project standard Internal control C is less than 0.180.13 ~ 0.17 Si is less than 0.550.15 ~ 0.25 Mn1.0 ~ 1.61.2 ~ 1.4 P = 0.025 is less than or less than 0.025, or 0.025, or 0.025, 0.015 ~ 0.015 ~ 0.025 Table 2 chemical components control % Table 4 impact test data after oil
30、 bath Oil bath temperature / ℃ 120150200280340-40 ℃ AkV/J42, 84421 0,18,8106,50,1020,128,4222,20,58 Test temperature Degree / ℃ The normal temperature 30-40 - Constant temperature of 7d1 # 10834322 # 13046133 # 10810144 # 14212105 # 138269 Room temperature of 1
31、5d1 # 10444462 # 11838183 # 9634404 # 11216385 # 1301820 Table 6. Time-temperature adverse impact data J Water bath time No bath 30 min45min60min90min The normal temperature 122,92,130116,144,114100,130,128128,120,12696,132,112-30 ℃ 46,24,4826,48,3028,20,1212,22,1
32、840,38,32-40 ℃ 26, 14, 2834, 40, 32, 18, 12, 18, 14, 14, 12, 16 Table 5 water bath after the impact test data JC0.178 Si0.214 Mn1.26 P0.009 S0.007 Cr0.024 Nb0.017 Ni0.01 Cu0.014 Al0.005 [O] * 10-654.1 [N] times 10-637.5 Table 3 samples of chemical composition and gas content % The
33、impact test data after oil bath is shown in table 4 (30min oil bath time). The test data of impact test after water bath is shown in table 5 (water bath temperature 100 ℃); Under normal temperature (10 ~ 30 ℃) aging impact test data shown in table 6. From a large number of experimental data, t
34、he temperature of normal temperature has a basic impact Is not affected, 15 d after aging, and 30 ℃ and 40 ℃ - impact sbent in Paris Improved, below 30 ℃ impact energy as a whole is not high and volatile, this master If it is caused by the release of residual stress; Oil bath or water bath
35、quickly The effect of effect on the impact work has not been significantly beneficial It is not obvious that the impact work under the temperature of temperature is not obvious To take a water bath or oil bath with the test specimen, and the condition of the permanent temperature of the who
36、le steel 40 Different ways of quick aging of oil bath or water bath are not desirable. Determination of temperature range of low temperature brittle transition temperature 3.1 low temperature brittleness curve In order to adjust the composition of Q345E steel, it is mainly to adopt he
37、alth C, Nb, control measures, such as P, S, O content can produce - 40 ℃ Impact work meets national standards, but it is difficult to operate. Its prone to volatility. In order to assess the current production conditions Q345E The low temperature impact performance of steel is measured i
38、n the laboratory Temperature change curve of low temperature brittleness of shape steel (see figure 1). From figure 1 It can be seen that the impact absorption work has two platforms on the curve of temperature change Platform for high shock absorption function part, when the temperature dr
39、opped to about 30 ℃, With the decreasing of temperature, AkV fell sharply, when the temperature dropped to 40 ℃ In the lower case, the AkV changes small and enters the lower platform of low impact absorption work. Akv/J - 80-80 Test temperature / ℃ FIG. 1 steel Q345EH section steel ak
40、v-t curve 3.2 macro fracture analysis The typical macroscopic fracture morphology of a series of temperature shocks is shown in FIG. 2, from the room In the process of temperature drop to - 70 ℃, impact sample from ductile to brittle fracture The transition of the sexual fracture, the ar
41、ea of the fiber area and the shear labial area gradually dwindled to eliminate The area of the crystalline region gradually expands to the whole section. 40 ℃ to - The lower crispy tendency is severe. Room temperature 0 ℃ to 30 ℃ and 40 ℃ Figure 2. Typical temperature impact of the steel
42、 Q345EH section steel 3.3 microfracture analysis The microcosmic fracture of the impact of temperature impact on the whole section is in a fortitude. It shows that the steel has high toughness; - 10 ℃ when fracture has heart The crystallization appears in the river pattern; The temperatu
43、re dropped to - 30 ℃, the knot The crystalline region has expanded to the bottom; To 40 ℃ when only small near the gap The region appears to have a tough fossa, while the rest of the region has a fluvial streak The levy. The microfracture morphology shows that the temperature of the test is
44、 reduced The fracture mechanism is gradually changed from the fracture of the ductile to cleavage fracture. The microfracture morphology of typical test temperature impact samples is shown in FIG. 3 Shown below. 100 mu m100 approximately mu m100 approximately mu m100 approximately micron
45、s At room temperature the core department - 30 ℃ to 10 ℃ heart heart department to 40 ℃ Room temperature near gap area - 10 ℃ near gap area - 30 ℃ near gap area to 40 ℃ near gap area FIG. 3 typical temperature impact microfracture morphology of steel Q345EH section steel 100 mu m100 appr
46、oximately mu m100 approximately mu m100 approximately microns The energy method determines the temperature of the low temperature of Q345EH steel Temperature range between 30 ~ 40 ℃ - -. Good - 30 ℃ when the impact energy And stable, below 30 ℃ impact energy fell sharply, and 40 ℃ impact en
47、ergy Overall poor performance, brittle fracture tendency is serious. You can see, by composition The whole, and 30 ℃ impact energy can guarantee, and below - 30 ℃ steel has entered Ductile to brittle transition zone, want to ensure a stable qualified to 40 ℃ impact energy is difficult Is
48、 very large. Therefore, to further reduce the brittle transition temperature, from the root To improve the quality of steel, other technical means should be considered. Low temperature impact work and analysis of the cause of fluctuation 4.1 metallographic analysis Some samples of metall
49、ographic tissue observed that ferrite/pearlite Q345E big h-beam and 40 ℃ low impact toughness of cause analysis Dong Changxing etc. 2009 41 Different ways of quick aging of oil bath or water bath are not desirable. Determination of temperature range of low temperature brittle transition
50、temperature 3.1 low temperature brittleness curve In order to adjust the composition of Q345E steel, it is mainly to adopt health C, Nb, control measures, such as P, S, O content can produce - 40 ℃ Impact work meets national standards, but it is difficult to operate. Its prone to vola
51、tility. In order to assess the current production conditions Q345E The low temperature impact performance of steel is measured in the laboratory Temperature change curve of low temperature brittleness of shape steel (see figure 1). From figure 1 It can be seen that the impact absorption wor
52、k has two platforms on the curve of temperature change Platform for high shock absorption function part, when the temperature dropped to about 30 ℃, With the decreasing of temperature, AkV fell sharply, when the temperature dropped to 40 ℃ In the lower case, the AkV changes small and enters
53、 the lower platform of low impact absorption work. Akv/J - 80-80 Test temperature / ℃ FIG. 1 steel Q345EH section steel akv-t curve 3.2 macro fracture analysis The typical macroscopic fracture morphology of a series of temperature shocks is shown in FIG. 2, from the room In the pro
54、cess of temperature drop to - 70 ℃, impact sample from ductile to brittle fracture The transition of the sexual fracture, the area of the fiber area and the shear labial area gradually dwindled to eliminate The area of the crystalline region gradually expands to the whole section. 40 ℃ to -
55、 The lower crispy tendency is severe. Room temperature 0 ℃ to 30 ℃ and 40 ℃ Figure 2. Typical temperature impact of the steel Q345EH section steel 3.3 microfracture analysis The microcosmic fracture of the impact of temperature impact on the whole section is in a fortitude. It shows t
56、hat the steel has high toughness; - 10 ℃ when fracture has heart The crystallization appears in the river pattern; The temperature dropped to - 30 ℃, the knot The crystalline region has expanded to the bottom; To 40 ℃ when only small near the gap The region appears to have a tough fossa, wh
57、ile the rest of the region has a fluvial streak The levy. The microfracture morphology shows that the temperature of the test is reduced The fracture mechanism is gradually changed from the fracture of the ductile to cleavage fracture. The microfracture morphology of typical test temperatur
58、e impact samples is shown in FIG. 3 Shown below. 100 mu m100 approximately mu m100 approximately mu m100 approximately microns At room temperature the core department - 30 ℃ to 10 ℃ heart heart department to 40 ℃ Room temperature near gap area - 10 ℃ near gap area - 30 ℃ near gap area to
59、 40 ℃ near gap area FIG. 3 typical temperature impact microfracture morphology of steel Q345EH section steel 100 mu m100 approximately mu m100 approximately mu m100 approximately microns The energy method determines the temperature of the low temperature of Q345EH steel Temperature range
60、 between 30 ~ 40 ℃ - -. Good - 30 ℃ when the impact energy And stable, below 30 ℃ impact energy fell sharply, and 40 ℃ impact energy Overall poor performance, brittle fracture tendency is serious. You can see, by composition The whole, and 30 ℃ impact energy can guarantee, and below - 30 ℃
61、steel has entered Ductile to brittle transition zone, want to ensure a stable qualified to 40 ℃ impact energy is difficult Is very large. Therefore, to further reduce the brittle transition temperature, from the root To improve the quality of steel, other technical means should be considere
62、d. Low temperature impact work and analysis of the cause of fluctuation 4.1 metallographic analysis Some samples of metallographic tissue observed that ferrite/pearlite Q345E big h-beam and 40 ℃ low impact toughness of cause analysis Dong Changxing etc. 2009 41 Shandong metallurgic
63、al volume 31, April 2009 AnalysisonReasonsofLowImpactToughnessat - 40 ℃ ofQ345EBigSizeH - beamDONGChang - xing, CHENGMei, SHIZhen - Ming, DONGBing - cheng, LIUHong - yan (LaiwuIronandSteelGroupCorporation Laiwu271104, China) Abstract:Abstract:TheageingtestsofQ345EbigsizeH-beamwerestudiedand
64、theresultsshowedthattheinfluenceofageingonthelowtemperatureimpacttoughnessat-40℃wasless.Thechangecurveofabsorbed-in-fractureenergywiththetemperaturewasconfirmedbyenergymethodanditsbrittletransitiontemperaturerangeisfrom-30℃to-40℃.Withmicroscopeandelectronprobeetc,themetallographicstructure,macrograp
65、handmicro-morphologyoftheimpactfractureandthemicro-morphologyandmicroareacompositionofinclusionwereanalyzed.Theresultsindicatedthatthemainreasonsoflowimpacttoughnessweretheseriouszonestructureandthenon-metallicinclusion. Keywords: Keywords: H - beam; Lowtemperatureimpacttoughness; Ageing; Zonestr
66、ucture; The inclusion The ribbon is more serious. The performance of steel is also larger Because of the microstructure of adjacent bands of banded tissue, it is affected The performance is also different, with low performance under external forces Exposure, and the stress concentration between the strong and weak bands, is made The overall mechanical properties were reduced and the anisotropy was obvious The method of overheat treatment to eliminate the test sample of banded
- 溫馨提示:
1: 本站所有資源如無(wú)特殊說(shuō)明,都需要本地電腦安裝OFFICE2007和PDF閱讀器。圖紙軟件為CAD,CAXA,PROE,UG,SolidWorks等.壓縮文件請(qǐng)下載最新的WinRAR軟件解壓。
2: 本站的文檔不包含任何第三方提供的附件圖紙等,如果需要附件,請(qǐng)聯(lián)系上傳者。文件的所有權(quán)益歸上傳用戶所有。
3.本站RAR壓縮包中若帶圖紙,網(wǎng)頁(yè)內(nèi)容里面會(huì)有圖紙預(yù)覽,若沒(méi)有圖紙預(yù)覽就沒(méi)有圖紙。
4. 未經(jīng)權(quán)益所有人同意不得將文件中的內(nèi)容挪作商業(yè)或盈利用途。
5. 裝配圖網(wǎng)僅提供信息存儲(chǔ)空間,僅對(duì)用戶上傳內(nèi)容的表現(xiàn)方式做保護(hù)處理,對(duì)用戶上傳分享的文檔內(nèi)容本身不做任何修改或編輯,并不能對(duì)任何下載內(nèi)容負(fù)責(zé)。
6. 下載文件中如有侵權(quán)或不適當(dāng)內(nèi)容,請(qǐng)與我們聯(lián)系,我們立即糾正。
7. 本站不保證下載資源的準(zhǔn)確性、安全性和完整性, 同時(shí)也不承擔(dān)用戶因使用這些下載資源對(duì)自己和他人造成任何形式的傷害或損失。
最新文檔
- 6.煤礦安全生產(chǎn)科普知識(shí)競(jìng)賽題含答案
- 2.煤礦爆破工技能鑒定試題含答案
- 3.爆破工培訓(xùn)考試試題含答案
- 2.煤礦安全監(jiān)察人員模擬考試題庫(kù)試卷含答案
- 3.金屬非金屬礦山安全管理人員(地下礦山)安全生產(chǎn)模擬考試題庫(kù)試卷含答案
- 4.煤礦特種作業(yè)人員井下電鉗工模擬考試題庫(kù)試卷含答案
- 1 煤礦安全生產(chǎn)及管理知識(shí)測(cè)試題庫(kù)及答案
- 2 各種煤礦安全考試試題含答案
- 1 煤礦安全檢查考試題
- 1 井下放炮員練習(xí)題含答案
- 2煤礦安全監(jiān)測(cè)工種技術(shù)比武題庫(kù)含解析
- 1 礦山應(yīng)急救援安全知識(shí)競(jìng)賽試題
- 1 礦井泵工考試練習(xí)題含答案
- 2煤礦爆破工考試復(fù)習(xí)題含答案
- 1 各種煤礦安全考試試題含答案